Imitation Cloisonn?/ Synthetic Enamel
Process: Copper stamped with imitation cloisonné / synthetic
enamel
Material: Copper
Enamel: Imitation Cloisonné / Synthetic Enamel
Thickness: Thickness is various depending on the size of
design.
Plating: Gold / Antique Gold / Silver / Antique Silver /
Nickel / Black Nickel / Antique Nickel / Copper / Antique Copper /
Brass / Antique Brass
Epoxy coating: Without
Attachment: Various
Color reference: Pantone Color Chart
STEP 1
Stamping Molding
Molds the metal surface to form the design.
STEP 2
Outline Cutting
Cutting molds are made separately, then cut to the exact outline of
the design. Outline cutting molds may be required depending on the
complexity of the design. If a center hole or cut-out is required,
an additional cut-through mold must be used.
STEP 3
Coloring
Synthetic enamel is carefully hand-filled, one color at a time,
using different sized syringes. Drying. To prevent defects, a high
degree of skill is required in order to keep each color and the
correct amount of enamel in the proper area.
STEP 4
Baking
The metal piece is baked at approximately 450F for 12 to15 minutes.
STEP 5
Stoning & Polishing
Wait until every piece has cooled. Finish the surface by stoning
with a carborundum stone until all excess color has been worn away.
Polish the surface until smooth and shining.
STEP 6
Attachment
Solder attachment onto the back of each piece.
STEP 7
Plating
Plating now can be processed. The quality of plating varies with the
length of time the metal is soaked in the plating liquid.
STEP 8
Inspection & Packing
All items are strictly inspected before delivery. Customer’s
satisfaction is guaranteed